A visiting artist to run a couple of workshops for us, but we really needed to explore the process more and find ways to enable our workshop members to be able to work independently in our space. Preferably with materials and equipment already compatible with what we have been using to etch copper plate. One stumbling block I found was the contradictory advice from different practitioners, plus I couldn’t fit in the time necessary to explore things fully within my allotted one day a week. So, when a modest amount of funding was found, I was able to put aside time for some research and development. And then I was able to put on a members’ only workshop to “stress-test” my theories and processes.
Here is a glimpse of the results on my Instagram
This is the BRIEF version of my R&D report…
Preliminary thoughts….
The aluminium typically used for etching is “mill-finished” – this means it’s the aluminium’s unaltered, raw surface as it leaves the rolling mill. This is the original state of aluminium, without any surface treatments like anodizing, painting, or lacquering. The surface is characterized by a slightly rough, matte texture. Aluminium forms a protective oxide film when exposed to air. This layer protects the metal beneath from further degradation. This may be useful in industry, but can cause issues with etching. If we were to do a simple hard ground etching using aluminium, the needle would be sufficient to break through the resistant oxide layer, but for open bite to emulate aquatint tones this microscopically thin oxide layer can result in uneven etching. Even to the point of minimal or no etching on an older plate that has been exposed to air for some time.

For etching, the beauty of etching aluminium is that it can be very immediate and lends itself to expressive, impactful mark-making. It is a much more “aggressive” etch than copper-plate and one of my aims is to exploit the differences to put space between the two processes. If people want controlled step by step processes more closely related to traditional etching, then copper would be the first choice. And if people would like something quickly and simply etched, then aluminium is a good choice.
Another aim is to settle on processes and materials that are compatible with the Acrylic Resist Etching with Copper & Ferric Chloride that we have been doing at Double Elephant for getting on for 30 years. Partly to save confusion for members who may like to try both metals, and also because of the lack of space to store extra materials.
Aluminium behaves differently to copper….
Aluminium is a granular, porous metal (one of the reasons why it is so light). The key point for this regarding etching is that no aquatint is required to create tone when etching open bite areas. But I also suspect that the porous nature makes it susceptible to contamination that might not be so easy to wash off (see issues with brasso below).
Aluminium can create a tough oxide skin very rapidly on exposure to air, especially in proximity with water. My research with different practitioners brings up contradictory opinions about this. Possibly, if people use better quality of aluminium with a protective film covering, and only remove the covering directly before processing the plate for etching, this may not be an issue. But as we tend to use budget metals and can have plates hanging around for a long time before etching, I believe (especially in the light of my experiments) that this an issue we should take into account when preparing any aluminium plate for etching.
For the experiments I focused on using latex masking fluid with pour on hard ground (Klear Floor Polish. Cleans up with soapy water, strip with Mystrol detergent). Some tests include needle marks, other potential lift grounds and marker pen as a resist.
Later tests also included our Soft/wet ground too.
EXPERIMENTS
There are details of 9 experiments in my full report….
Having purchased some very cheap, thin aluminium online, I started my experiments with the materials I had to hand. I had ordered some finer sandpaper, but this hadn’t arrived at the point I started. It bothers me having to sand the surface of an etching plate. I don’t do this with Acrylic Resist Etching on copper (despite initial instructions from the Edinburgh Etch process said to do so). But because I have been finding that dipping the copper plates in our stripper to give them an initial clean to be useful (roofing copper often having baked on oil to stop tarnish and therefore making it harder to degrease). I thought it would be worth seeing if this would also have a beneficial effect on the aluminium too.

Experiments contrasted sanding and not sanding; varying fineness of grit sanding, plus wet & dry; brasso to bring back shine, degrease and not degrease; semi permeable resists to add texture to open bite and touched upon alternative lift grounds; and other grounds..
I suspect that brasso may cause more problems than it solves. Perhaps the porous nature of the metal makes basso contaminants hang on and not wash away with the degreaser? Possibly in that case our strong degreaser might also be clinging on too? (It’s notable with the copper plate that the degreaser needs to be thoroughly washed off. If anyone leaves a residue on the plate grounds might not adhere properly.)
Overall conclusions.
Sanding is necessary with sufficient grittiness (2000 grit) to break through any resistant oxide surface (necessary for a good open bite etch). This benefits from polishing with wet & dry finer grits to bring back as much smoothness as you can. Don’t degrease unless necessary (I need further experiments with alternative degreasers).
If you are doing a simple lift ground with pour on hard ground you may consider leaving the ground on for maximum brightness to the highlights. I have yet to stress test this to see how long it lasts.
The use of soft/wet ground has a vast amount of mark-making potential. I also experimented with ways of applying different ground in order to do a simple etch rather than etching with several steps.
A good way of achieving brighter highlights is to use extender in the etching ink. With good rich blacks etched with open bite, there is plenty of potential for achieving good prints with extender. Black ink can hold its own with 2/3 or more of extender. Other colours would vary depending on the particular pigments. More experimentation potential.
Note – I’ve not conducted etching time experiments so far. Clearly this will vary with the strength and age of the solution. We have small scraps of aluminium that are useful for strength testing. These need a quick rubdown with sandpaper before use otherwise they don’t etch much at all.